HOME > Products > Insulating material / Industrial plastic > Thermosetting resin laminates /Line-ups
> Paper/Phenolic laminates(Thick plate) PS-1126(PL-PEM/XX)
Paper/Phenolic laminates(Thick plate) PS-1126(PL-PEM/XX)
Test items |
Unit |
Treatment |
PS-1126 |
Electrical strength
(Vertical to layer) |
In oil 1 min. |
MV/m |
C-90/20/65 |
13 OK (13<) |
Breakdown voltage
(Vertical to layer) |
In oil 1 min. |
MV/m |
C-90/20/65 |
30~40 |
Electrical strength
(Parallel to layer) |
In hot oil |
kV |
O-0.5/90 |
8 OK (8 <) |
Breakdown voltage
(Parallel to layer) |
In hot oil |
kV |
O-0.5/90 |
15~20 |
Insulation resistance |
at RT |
MΩ |
C-90/20/65 |
104~105 (5X102<) |
After heat treatment |
C-90/20/65
+D-2/100 |
10~102 (10<) |
Volume resistivity |
at RT |
MΩ-cm |
C-90/20/65 |
5×105~107 |
After moisture treatment |
C-90/20/65
+C-96/40/90 |
|
Surface resistance |
at RT |
MΩ |
C-90/20/65 |
5×102~103 |
After moisture treatment |
C-90/20/65
+C-96/40/90 |
|
Dielectric constant
(1MHz) |
at RT |
- |
C-90/20/65 |
4.5~5.5 |
After dipping treatment |
C-90/20/65
+D-24/23 |
|
Dissipation factor
(1MHz) |
at RT |
- |
C-90/20/65 |
0.035~0.055 |
After dipping treatment |
C-90/20/65
+D-24/23 |
|
Flexural strength |
Vertical to layer |
MPa |
A |
150~240 (98<) |
Parallel to layer |
- |
Compressive strength |
Vertical to layer |
MPa |
A |
275~330 |
Parallel to layer |
175~230 |
Tensile strength |
MPa |
A |
100~180 |
Izod impact strength |
Parallel to layer |
J/cm |
A |
0.29~0.39 (0.20<) |
Cleavage strength |
kN |
A |
4.3~5.3 (3.4<) |
Rockwell hardness |
|
- |
A |
M.105~115 |
Water absorption |
1.6mm thick |
% |
E-24/50 +D-24/23 |
|
3.0mm thick |
E-24/50 +D-24/23 |
(1.30>) |
10mm thick |
E-24/50 +D-24/23 |
0.3~0.5 (0.85>) |
Appearance after heating treatment |
2 hours |
℃ |
A |
130 OK (130℃) |
Specific gravity |
- |
A |
1.34~1.40 (1.25-1.50) |
Acetone resistance |
- |
A |
OK (OK) |
|
*The above figures show the standard properties and guaranteed value is showed in parentheses
*Test method : JIS K-6911
*Treatment condition
A=Accepted state, C=Constant Temperature and humidity , D=Dipping in water E=Electric heating , O=Oil dipping
Starting from the left figures show Time(h)/Temeperature(℃)/Humidity(%) |
Specifications and dimension
Thickness(mm) |
8~20 |
Standad dimension
(mm) |
1000×1000 |
◯ |
1000×1200 |
◯ |
1000×1500 |
|
1000×2000 |
◯ |
1200×2000 |
◯ |
Thickess
tolerance
(mm) |
|
|
0.5 |
|
0.6 |
|
0.8 |
|
1.0 |
|
1.2 |
|
1.5 |
|
1.6 |
|
2.0 |
|
2.5 |
|
3.0 |
|
4.0 |
|
5.0 |
|
6.0 |
|
8.0 |
±0.40 |
10.0 |
±0.45 |
12.0 |
±0.50 |
15.0 |
±0.55 |
16.0 |
±0.60 |
18.0 |
±0.70 |
20.0 |
±0.70 |
25.0 |
|
30.0 |
|
35.0 |
|
400 |
|
50.0 |
|
75.0 |
|
100.0
|
|
|
*Minimum quantity of order would be quoted according to product |